What Is GCr15 Steel?

GCr15 is the world’s most important bearing steel, accounting for over 90% of all rolling element bearing production globally. Designated under Chinese standard GB/T 18254, GCr15 is a high carbon chromium steel containing C 0.95–1.05% and Cr 1.40–1.65% — a hypereutectoid composition specifically engineered to achieve extreme hardness (HRC 61–65 after quenching and tempering) with superior wear resistance and dimensional stability for rolling contact applications.

The designation: G = Gun (滚, rolling in Chinese, referring to rolling bearings), Cr = chromium, 15 = chromium content approximately 1.5% (×10 of percentage). GCr15 is equivalent to AISI 52100 (USA), SUJ2 (Japan), 100Cr6 / 1.3505 (Europe) — all describing the same fundamental alloy used by every major bearing manufacturer worldwide including SKF, NSK, NTN, FAG, Timken and NACHI.

Unlike structural and alloy steels where tensile strength and yield are the primary acceptance criteria, GCr15 quality is judged by hardness, non-metallic inclusion content, carbide uniformity and decarburization — the parameters that directly determine bearing fatigue life under millions of rolling contact cycles.

Chemical Composition — GCr15 (GB/T 18254) vs Equivalents

ElementGCr15 (GB)52100 (ASTM)100Cr6 (EN)SUJ2 (JIS)
C0.95–1.050.98–1.100.93–1.050.95–1.10
Cr1.40–1.651.30–1.601.35–1.601.30–1.60
Mn0.25–0.450.25–0.450.25–0.45≤0.50
Si0.15–0.350.15–0.350.15–0.350.15–0.35
P max0.0250.0250.0250.025
S max0.0250.0250.0150.025
Ni max0.300.250.300.25
Cu max0.250.300.300.25
Mo max0.100.080.10—
O max (ppm)≤12–15≤15≤15≤15
Ti max (ppm)≤30———

All four designations describe the same fundamental alloy: ~1% C + ~1.5% Cr. GCr15 uniquely specifies Ti limit (≤30 ppm) — TiN inclusions are the MOST damaging inclusion type for bearing fatigue.

Why ~1% Carbon + ~1.5% Chromium?

ElementRolePractical Benefit
Carbon (1.0%)Hypereutectoid — provides excess carbon for chromium carbide formation and extreme martensite hardnessHRC 61–65 after Q&T. Hard carbide particles provide microscopic “armor” against wear.
Chromium (1.5%)Forms hard Cr₇C₃ and Cr₂₃C₆ carbides. Increases hardenability for through-hardening.Through-hardens bearing components up to ~30mm wall. Superior wear and fatigue resistance.

Properties — Annealed vs Q&T

ConditionPurposeHardnessTensile (approx.)Microstructure
Annealed (delivery)Machining — turning, grinding, drillingHB ≤207 (HRC ≤15)~680 MPaSpheroidized pearlite + spherical carbides
As-QuenchedIntermediate — before temperingHRC 63–66—Martensite + retained austenite + undissolved carbides
Q&T 170°C (bearing)Standard bearing serviceHRC 61–63~2000+ MPa (compressive)Tempered martensite + fine carbides
Q&T 200°CModerate bearingHRC 60–62—Tempered martensite
Q&T 300°CShafts needing hardness + toughnessHRC 55–58~1500 MPaTempered martensite
Q&T 400°CCam followers, moderate wearHRC 48–55~1200 MPaTempered martensite

GCr15 is delivered ANNEALED for machining. End user performs Q&T to achieve service hardness. Temper temperature determines final hardness: lower temper = harder = more wear resistant = less tough.

Critical Quality Parameters — Why Bearing Steel Is Different

ParameterBearing Steel (GCr15)Structural Steel (42CrMo)Why Different
Primary acceptanceInclusions + Carbide + Decarb + HardnessTensile + Yield + ImpactBearing life depends on cleanliness, not tensile
Oxygen limit≤12–15 ppm (VD required)Not typically specifiedO forms oxide inclusions → fatigue cracks
Titanium limit≤30 ppmNot specifiedTiN = most damaging inclusion type
Inclusion ratingASTM E45 — mandatory, strict limitsRarely testedInclusions initiate rolling contact fatigue
Carbide networkRated per GB/T 18254Not applicableNetwork carbide = non-uniform hardening
DecarburizationMeasured, strict limitsRarely specifiedDecarb = soft surface = early bearing failure
Service hardnessHRC 61–65HRC 28–34Bearing needs extreme hardness for contact life

Oxygen and Titanium — Why ppm Matters

Bearing failures almost always start at non-metallic inclusions inside the steel:

  • Oxygen forms alumina (Al₂O₃) and silicate inclusions — hard, brittle particles that act as stress concentrators under rolling contact, initiating micro-cracks that grow into spalls (surface flaking).
  • Titanium forms titanium nitride (TiN) — the MOST damaging inclusion type. TiN is extremely hard (~2000 HV), angular shape, cannot be deformed during rolling, and creates severe stress concentration. Even a single large TiN particle can initiate fatal bearing failure.

Lower O and Ti = fewer inclusions = longer bearing life. Premium bearing steel has O ≤10 ppm and Ti ≤15 ppm. Standard grade: O ≤15 ppm, Ti ≤30 ppm.

Inclusion Rating — ASTM E45

Inclusion TypeExampleStandard BearingPremium Bearing
Type A (Sulfide)MnS stringers≤2.0≤1.5
Type B (Alumina)Al₂O₃ clusters≤2.0≤1.5
Type C (Silicate)Glass-like silicate≤1.0≤0.5
Type D (Globular oxide)Round oxide particles≤1.0≤0.5

Inclusion rating is a PRIMARY acceptance criterion for bearing steel — equivalent in importance to tensile strength for structural steel.

Carbide Network and Banding

After solidification, the excess carbon and chromium form a continuous carbide network along grain boundaries. This network is hard and brittle — if not broken down during hot working and annealing, it causes:

  • Non-uniform hardness after hardening
  • Reduced toughness — crack initiation at carbide network
  • Premature bearing failure

Hot rolling and spheroidize annealing (700–740°C, 15–25 hours) break the network into uniformly dispersed spherical carbides — the optimal microstructure for machining and subsequent hardening. Carbide network rating per GB/T 18254 is a critical acceptance parameter.

Heat Treatment Guide

StepTemperatureTimeCoolingResult
1. Austenitizing830–845°C30–60 min soak—Dissolves sufficient C into austenite
2. Oil Quench→ 60–80°C oilUntil cooledOil quenchHRC 63–66 (martensite + retained austenite)
3. Tempering150–180°C2 hoursAir coolHRC 61–63 (bearing standard)
4. Cold Treatment (optional)-70 to -80°C2 hoursReturn to room tempTransforms retained austenite → dimensional stability

Critical: Austenitizing temperature must be precisely controlled. Too low (≤820°C): insufficient carbon dissolves → low hardness. Too high (≥860°C): excessive grain growth → reduced fatigue life + excessive retained austenite. The 830–845°C window is narrow and critical for bearing performance.

GCr15 Grade Family

Grade (GB)C%Cr%SpecialApplication
GCr150.95–1.051.40–1.65StandardStandard bearing — 90%+ of production
GCr15SiMn0.95–1.051.40–1.65Si 0.40–0.70, Mn 0.90–1.20Large bearing rings (better hardenability)
GCr15SiMo0.95–1.051.40–1.65Si + Mo 0.10–0.25Very large bearings (maximum hardenability)
GCr40.95–1.050.35–0.65Lower CrSmall bearings (economy)

Comparable Grades — Cross-Reference Table

StandardGradeKey Note
GB/T 18254 (China)GCr15Chinese primary standard. Specifies Ti limit uniquely.
ASTM A295 (USA)52100 (UNS G52986)American equivalent. AISI/SAE designation.
EN ISO 683-17 (Europe)100Cr6 / 1.3505European equivalent. EN designation system.
JIS G 4805 (Japan)SUJ2Japanese equivalent. Dominant in Asian bearing industry.
DIN 17230 (Germany)100Cr6Historical German, now EN.
BS 970 (UK)535A99British equivalent (historical).
SKF / NSK / NTN / FAGInternal specsMajor bearing OEMs use 52100/SUJ2/100Cr6 with additional internal quality specs.

Note: All designations describe the same alloy: ~1% C + ~1.5% Cr. Differences between standards are minor (trace element limits, testing methods). The fundamental metallurgy is identical worldwide.

Available Product Forms

ProductSpecificationApplication
GCr15 Bearing Steel BarØ10–300mm, annealed/turned/groundBearing rings, races, shafts, rollers

Also available: GCr15 wire rod (Ø5.5–25mm) for ball and roller cold heading production.

Applications

  • Ball bearings — balls, inner/outer races, cages for all sizes and types
  • Roller bearings — cylindrical, tapered, spherical, needle rollers and races
  • Precision shafts — spindle shafts, pump shafts, instrument shafts requiring hardness + wear resistance
  • Linear motion — linear guide rails, linear bearing shafts, ball screws
  • Automotive — wheel hub bearings, transmission bearings, differential bearings
  • Industrial — motor bearings, gearbox bearings, conveyor bearings, pump bearings
  • Aerospace — aircraft wheel bearings, engine auxiliary bearings, instrument bearings
  • Machine tools — spindle bearings, ball screw support bearings
  • Railway — axle bearings, traction motor bearings
  • Mining — crusher bearings, vibrating screen bearings, conveyor idler bearings
  • Precision instruments — watch components, measuring instrument pivots
  • Wear-resistant components — cam followers, rocker arm pivots, valve train components

Beyond Bearings — Other GCr15 Applications

GCr15’s extreme hardness (HRC 61–65) and superior wear resistance make it suitable for non-bearing applications:

  • Linear guide rails — precision CNC machine guide surfaces
  • Ball screw shafts — precision lead screw shafts for CNC
  • Gauges and measuring tools — plug gauges, ring gauges, inspection pins
  • Cold work tooling — small punches, dies for limited production runs
  • Wear-resistant pins and bushings — in wear-critical assemblies

Note: GCr15 has LOW toughness at service hardness (HRC 61–65) — NOT suitable for impact-loaded applications. For impact + hardness, use 42CrMo Q&T at HRC 28–34.

Decarburization — Critical for Bearing Surface

The bar surface must NOT lose carbon during hot rolling or heat treatment. Decarburization creates a soft surface layer that dramatically reduces bearing fatigue life:

  • Soft surface under rolling contact → plastic deformation → rapid wear → early failure
  • Surface hardness must match core hardness for uniform contact stress distribution
  • Total and partial decarburization limits strictly controlled per ASTM A295 / GB/T 18254

GCr15 MTC reports decarburization depth — a critical acceptance parameter alongside inclusion rating and carbide quality.

Frequently Asked Questions

What is GCr15?

GCr15 is a high carbon chromium bearing steel (C 0.95–1.05%, Cr 1.40–1.65%) designed for rolling element bearings. After quenching and tempering, it achieves HRC 61–65 — providing exceptional wear resistance and contact fatigue life. Equivalent to AISI 52100, SUJ2, 100Cr6. Accounts for >90% of global bearing production.

What is the AISI equivalent of GCr15?

AISI 52100 (UNS G52986). Both have ~1% C and ~1.5% Cr. Other equivalents: SUJ2 (JIS), 100Cr6/1.3505 (EN). All are the same fundamental alloy used by every major bearing manufacturer worldwide.

Why are oxygen and titanium so important?

Oxygen forms oxide inclusions that initiate fatigue cracks under rolling contact. Titanium forms TiN — the most damaging inclusion type (extremely hard, angular, cannot deform). Lower O and Ti = fewer inclusions = longer bearing life. Premium GCr15 has O ≤10 ppm, Ti ≤15 ppm. Standard: O ≤15 ppm, Ti ≤30 ppm.

What delivery condition should I order?

Spheroidized Annealed: HB ≤207. Standard delivery for 95% of orders. Soft enough for machining (turning, grinding, drilling). End user then Q&T to service hardness.
Hot Rolled (Black): As-rolled with scale. For customers who will anneal themselves.
Turned/Ground: Precision surface + close tolerance. Premium cost but ready for final machining.

What heat treatment does GCr15 need?

End user performs: (1) Austenitize 830–845°C; (2) Oil quench; (3) Temper 150–180°C for bearings (HRC 61–63) or 200–300°C for shafts (HRC 55–62); (4) Optional cryogenic -70°C for dimensional stability. Temperature control is critical — ±10°C can significantly affect properties.

What is carbide network rating?

After solidification, excess C and Cr form carbide network along grain boundaries. This network must be broken by hot rolling + spheroidize annealing. Carbide network rating (per GB/T 18254) measures residual network: ≤2.5 for small bars, ≤3.5 for large bars. Lower = better = more uniform hardening.

Can GCr15 be welded?

Welding GCr15 is NOT recommended. At ~1% carbon, GCr15 has extremely high carbon equivalent and extreme HAZ hardening risk — virtually guaranteed to crack. For bearing assemblies requiring joining, use mechanical fastening (press fit, interference fit, retaining compounds) or design bearing seats separately from welded structure.

What is the MOQ?

5 MT per diameter for mill orders. 1 MT from stock. GCr15 is commonly stocked in Ø20–100mm spheroidized annealed round bar. Wire rod (Ø5.5–25mm for cold heading) also available.

Get Your GCr15 Bearing Steel Quote

Rigang Materials supplies GCr15 bearing steel bar from China’s specialized bearing steel mills with comprehensive quality documentation: oxygen content (ppm), inclusion rating (ASTM E45), carbide network/banding rating, decarburization depth and hardness. Multi-standard certification (GCr15 + 52100 + SUJ2 + 100Cr6) available.

📩 Request Quote    View Special Steel Products

💬 📞 ✉ 📋 ↑